Product Features Mix ratio (pbw) Pot life, 100 g (min / °F) Viscosity (cps / ËšF) Gel time
( min. / ËšF )
Cure cycle (time / ËšF) Tg (DSC) (ËšF) Flexural Strength (kpsi) Tensile Strength (kpsi)
Araldite LY 1556 / Aradur 42 Intermediate temperature use Short pot life 100 / 23 120 – 180 1,900 / 77 20 / 176 1 h / 248
+ 2 h / 302
298 – 316 18.9 €“ 19.7 8.9 €“ 10.4
Araldite LY 1556 / Aradur 917 / Accelerator DY070 Intermediate temperature use Anhydride system 100 / 90 /1 95 h / 77 700 / 77 150 / 176
11 / 248
4 h / 176
+ 4 h / 302
302 – 310 18.1 – 19.6 12.0 – 13.5
Resin XU 3508 / Aradur 917 / Accelerator DY 070 Intermediate temperature use Toughened Anhydride system 100 / 90 /1 105 h / 77 640 / 77 9 / 248
3 / 284
4 h / 176
+ 4 h / 284
275 – 293 20.3 €“ 21.8 10.9 €“ 11.6
Araldite LY 1564 / Aradur 2954 Intermediate temperature use 100 / 35 480 €“ 600 / 77 600 / 77 35-45 /176
16-18 / 212
3-4 / 284
2 h / 212
+ 2 h / 320
266 – 284 18.0 €“ 19.1 10.9 €“ 11.6
Araldite LY 1556 / Aradur 906 / Accelerator DY 070 High temperature Anhydride system 100 / 95 / 1 50 €“ 55 h / 77 2000 / 77 14-16 / 248 2 h / 248
+ 8 h / 320+
2 h / 356 N/A
RenLam LY 5210 / Aradur 2954 High temperature 100 / 53 7 €“ 9 h / 77 650 €“ 850 / 77 70-80 / 176
25-30 / 212
9-13 / 248
2 h / 176
+ 2 h / 320+
4 h / 356 N/A 435 €“ 471
Araldite LY 5210 / Aradur 3473 Very high temperature resistance 100 / 38 1200 – 1400 1,150 €“ 1,350 75-90 / 248
23-29 / 300
9-11 / 350
2 h / 212 +2 h / 284 +2 h / 400 501
Resin XB 9721 / Aradur 3473 High temperature Excellent hot/wet properties 100 / 38 80- 95 h 14000 / 77 35-45 / 284
18-21 / 320
8-11 / 356
2h / 176
+ 2h / 284+
2 h / 356+ 2 h / 420 499 €“ 529